SKS4 SKS4 chrome silicon steel is based on adding a certain amount of tungsten and the formation of the steel, because the quenching of tungsten help save more fine grain, leaving the tempering condition to obtain high toughness. SKS4 than 4CrW2Si steel and steel with high quenching hardness 5CrW2Si steel and some high-temperature strength. To withstand shock loads typically used in the manufacture of high wear resistance but requires tools such as pneumatic tools, chisels and punch Bureau mold, cold shear blades, punch with the die edge, pneumatic hammers and other tools.
Chemical composition SKS4 chemical composition of steel
C | Si | Mn | Cr | W | P | S |
0.55~0.65 | 0.50~0.80 | ≤0.40 | 1.00~1.30 | 2.00~2.70 | ≤0.030 | ≤0.030 |
Physical properties
SKS4 critical temperature of steel
Critical point | Ac1 | Ac3 | Ms |
Temperature (approximate) / ℃ | 775 | 810 | 280 |
SKS4 the thermal processing of steel SKS4 thermal processing
SKS4 the thermal processing of steel
SKS4 thermal processing Item | Heating temperature / ℃ | Before forging temperature / ℃ | Final forging temperature / ℃ | 冷却方式 |
Steel ingot Steel billet |
1170~1200 1150~1170 |
1150~1180 1100~140 |
≥850 ≥850 |
缓 冷 缓 冷 |