Spring steel
Position:Home >> Products >> Spring steel
China 4crW2Si
Public Time:2011年05月13日 | Sort:Spring steel | Hits:1015

Physical properties
4CrW2Si critical temperature of steel is shown in Table 2-17-2.
4CrW2Si critical temperature of steel
  
Critical point Ac1 Ac3 Ms
Temperature (approximate) / ℃ 780 840 315

Chemical composition

4CrW2Si steel chemical composition shown in Table 2-17-1.

  4CrW2Si steel chemical composition (GB/T1299-2000) w /%
  
C Si Mn Cr W P S
0.35~0.45 0.80~1.10 ≤0.40 1.00~1.30 2.00~2.50 ≤0.030 ≤0.030
Thermal processing
4CrW2Si steel thermal processing are shown in Table 2-17-3.
4CrW2Si steel thermal processing
  
Project Heating temperature / ℃ On forging temperature / ℃ Final forging temperature / ℃ Cooling
Ingot 
Billet
1180~1220
1150~1180
1150~1180
1100~1140
≥850
≥800

Slow cooling

Slow cooling